17-4 PH Studs
17-4 PH Studs are made from a precipitation hardened stainless steel most known for its exceptional strength and its ability to maintain its mechanical properties to 600°F. Compared to 316 stainless steel, 17-4 PH studs yield strength is up over 4 times greater. When compared to Duplex 2205 studs, the yield strength of 17-4 PH can be up to 2-½ times greater.
17-4 Studs are available in 8 different aged (precipitation hardened) conditions offering a variety of mechanical properties (see below). In addition,Raychin offers 17-4PH studs per ASTM F593 Grade 660 to ensure specific yield and tensile strengths for sensitive applications.
An extremely strong precipitation hardened stainless steel
· Well suited for high strength applciaitons
· Up to 4x stronger than 316 stainless steel
· Maintains its mechanical strength up to 600°F
· 17-4PH Chemistry & Specifications
· ASTM F593, Grade 630 fasteners
· 17-4PH Datasheet
17-4 PH Fastener Types: Studs, Threaded Rods
17-4PH Chemistry & Specifications
17-4PH Specifications: UNS S17400, AISI 630, ASTM A564-630, Werkstoff 1.4542, AMS 5604 Sheet, Strip and Plate, ASTM A 693 Plate
17-4PH | Fe | Cr | Ni | Cu | Mn | Si | Mo | Nb+Ta | C | P | S |
Min% |
| 15.0 | 3.0 | 3.0 | - | - | - | - | - | - | - |
Max% | Bal | 17.5 | 5.0 | 5.0 | 1.0 | 1.0 | 0.50 | 0.45 | 0.07 | 0.04 | 0.03 |
ASTM F593, Grade 630
This specification covers seven groups of stainless steel alloys, with ASTM F593, Grade 630 applying 17-4PH. ASTM F593 Grade 630 covers the requirements for 17-4PH stainless steel bolts, hex cap screws, and studs sized 0.25 to 1.50 inches, inclusive, in nominal diameter. It is intended for common use and for service applications requiring general corrosion resistance.
| Full-Size Tests | Machined Specimen Tests |
Stainless Steel Alloy Group | Condition | Alloy Mechanical Property Marking | Nominal Diameter (inches) | Tensile Strength (ksi) | Yield Strength (ksi) | Rockwell Hardness | Tensile Strength (ksi) | Yield Strength | Elongation % |
7(630) | AH | F593U | 1/4 to 1.5 IN | 135 to 170 | 105 | C28 to38 | 135 | 105 | 16 |
Common 17-4 Fastener Conditions: Aged Conditions vs Tensile Strength
Aged Condition | Ultimate Tensile (ksi) | Yield Strength at0.2% Offset (ksi) | Elongation% | Hardness Rc |
H900 | 200 | 185 | 14 | 40-47 |
H925 | 190 | 175 | 14 | 38-45 |
H1025 | 170 | 165 | 15 | 35-42 |
H1075 | 165 | 150 | 16 | 33-39 |
H1100 | 150 | 135 | 17 | 32-38 |
H115C | 145 | 125 | 19 | 28-37 |
H1150-M | 125 | 85 | 22 | 26-36 |
Annealed | 160 | 145 | 5 | ~35 |